Post by GatorGirl »

Just curious if anyone can tell me what trick to use to keep glass from sliding off of a face mold prior to and during fusing? The nose just seems to get in the way. Any info. would be greatly appreciated! ]
(*,)
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Post by Brock »

Try and balance it on the nose and the forehead, or, support a band of glass that crosses your mold with kiln furniture on the sides. Remove the furniture at the appropriate time. Brock
My memory is so good, I can't remember the last time I forgot something . . .
Brad Walker
Site Admin
Posts: 1544
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Post by Brad Walker »

Prop it on kiln furniture set on each side of the mold, about an inch or so above the nose. The glass will slump onto the nose first. Watch it, then remove the furniture as soon as it starts to drape over the nose. Then increase the temp a bit and let it finish the job. The chin usually takes the longest to slump.

And make sure you kilnwash the kiln furniture.
Linda Hassur
Posts: 44
Joined: Sat Mar 15, 2003 10:40 pm

folding glass on face

Post by Linda Hassur »

I've had problems with the glass folding somewhere between the chin and ear. Everything went OK except for the fold of glass. Would the kiln furniture prevent that from happening as I just balanced the glass on the nose. Thanks Linda
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Re: folding glass on face

Post by Brock »

Linda Hassur wrote:I've had problems with the glass folding somewhere between the chin and ear. Everything went OK except for the fold of glass. Would the kiln furniture prevent that from happening as I just balanced the glass on the nose. Thanks Linda
If you're making a mask, you should just slump some thin float, to define what actual shape your blank should be. Refine it by observing the results and cutting/trimming away excess glass from the shape of the original blank for the next try. It took me several attempts to get the shape I needed for a torso blank, but now I have a template I can use forever.

If you use the band technique, it seems to work okay, you probably won't get a lot of details off the side of the mold, but the face will work. Brock
My memory is so good, I can't remember the last time I forgot something . . .
GatorGirl
Posts: 38
Joined: Wed Jan 21, 2004 4:14 pm
Location: Germany

Post by GatorGirl »

I feel so enlightened about the information provided by everyone. I will give it a try ASAP. Thanks again!!!!

Kim
Jeri D
Posts: 65
Joined: Fri Mar 28, 2003 8:43 pm
Location: Martha's Vineyard.MA

Post by Jeri D »

What are the alternatives if you are:
1) Chicken about lifting the lid of the Jen ken when that hot
2) Chicken because I don't have a fireproof hood
3) Chicken because I would like to keep my hair thank you

Clucking girl Jeri
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Post by Brock »

Jeri Dantzig wrote:What are the alternatives if you are:
1) Chicken about lifting the lid of the Jen ken when that hot
2) Chicken because I don't have a fireproof hood
3) Chicken because I would like to keep my hair thank you

Clucking girl Jeri
1) Assistants
2) Assistants
3) Assistants
4) Make something else

Brock
My memory is so good, I can't remember the last time I forgot something . . .
Brad Walker
Site Admin
Posts: 1544
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Post by Brad Walker »

Jeri Dantzig wrote:What are the alternatives if you are:
1) Chicken about lifting the lid of the Jen ken when that hot
2) Chicken because I don't have a fireproof hood
3) Chicken because I would like to keep my hair thank you

Clucking girl Jeri
More beef!

Well, you can leave the glass just on the edge of the kiln furniture and pray that when it droops over the mold it slips off the furniture and manages to conform to the mold without hitting the sides of the furniture or messing things up.

It's a gamble, but then it's probably a gamble being a chicken in a world full of meat-eaters.
Jeri D
Posts: 65
Joined: Fri Mar 28, 2003 8:43 pm
Location: Martha's Vineyard.MA

Post by Jeri D »

:oops:
Well, I feel plucked. And Damn, I just found casting material to make some faces, and heck, with my size , I could fit a me in the kiln. Guess I'll have to grab a leg of venison and chew on that for awhile to toughen up . No sympathy on this site :lol:

going atkins jeri
Mark Kemp
Posts: 59
Joined: Mon Mar 10, 2003 11:57 am
Location: Corvallis, Oregon
Contact:

Post by Mark Kemp »

Jeri Dantzig wrote:What are the alternatives if you are:
1) Chicken about lifting the lid of the Jen ken when that hot
2) Chicken because I don't have a fireproof hood
3) Chicken because I would like to keep my hair thank you

Clucking girl Jeri
I wouldn't think you'd need a fireproof hood. Just keep your face back when you first open it, to let the blast of hot air escape (like you do with an oven baking chicken, if you remember....), then don't get your face closer than you need to. And keep your hair tied back -- it makes the chicken hard to chew. Protect your hands, though.
Find peace in your heart.

www.azurefire.etsy.com
GatorGirl
Posts: 38
Joined: Wed Jan 21, 2004 4:14 pm
Location: Germany

Post by GatorGirl »

I´ll be using my front loading kiln and some common sense for this project. It is definitely doable.

Kim
Lauri Levanto
Posts: 270
Joined: Tue Mar 11, 2003 7:33 am
Location: Halikko, Finland

Post by Lauri Levanto »

As a sculptor I got interested in slumping face mask.
Isn't it easier to slum *into* mold instead of over it?
What are the pros and cons?

-lauri
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Post by Brock »

lauri wrote:As a sculptor I got interested in slumping face mask.
Isn't it easier to slum *into* mold instead of over it?
What are the pros and cons?

-lauri
I don't think slumping into is any easier, and you'll get mold texture on the "face" of your face. Brock
My memory is so good, I can't remember the last time I forgot something . . .
Lauri Levanto
Posts: 270
Joined: Tue Mar 11, 2003 7:33 am
Location: Halikko, Finland

Post by Lauri Levanto »

The background for my question is

that I slumped 3/4 thick glass *over* a ceramic mold
(because I wanted the face (=mold marks) on the back.
On both attempts the glass broke over the midline of the face. Glass contracts more than ceramics.

-lauri
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Post by Brock »

lauri wrote:The background for my question is

that I slumped 3/4 thick glass *over* a ceramic mold
(because I wanted the face (=mold marks) on the back.
On both attempts the glass broke over the midline of the face. Glass contracts more than ceramics.

-lauri
I've slumped over ceramic face masks often. I really don't think that there is a general rule of thumb about slumping into or over, steel or cdramic. Success, in my opinion, is particular to the molds shape, not it's composition. Brock
My memory is so good, I can't remember the last time I forgot something . . .
Terry Ow-Wing
Posts: 124
Joined: Sun Mar 09, 2003 3:21 pm
Location: San Francisco, Ca.
Contact:

Re: Slumping Glass/Face Molds

Post by Terry Ow-Wing »

can someone post the make and model number of any ceramic mask that were easy to slump over? :D I would like to try out some of my "portrait" designs in a mask format. THanks!
Terry Ow-Wing Designs
Kilnformed and Lampworked Glass Art
http://GlassArt.weebly.com
Image
Jerrwel
Posts: 129
Joined: Thu Feb 10, 2005 6:25 pm
Location: Charlotte, NC

Re:

Post by Jerrwel »

Brad Walker wrote:Prop it on kiln furniture set on each side of the mold, about an inch or so above the nose. The glass will slump onto the nose first. Watch it, then remove the furniture as soon as it starts to drape over the nose. Then increase the temp a bit and let it finish the job. The chin usually takes the longest to slump.

And make sure you kilnwash the kiln furniture.
I'm wondering....is it possible to use a broader-based support (like a triangle or a cone) attached to stainless steel wire put through an observation hole and to pull the support from under the glass from outside the kiln as the glass starts to drape over the nose? Watch out, that wire may be hot!!! So many thoughts, so little time to experiment. The thought of working in a hot kiln literally scares the hell out of me!
Jerry
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: Slumping Glass/Face Molds

Post by Bert Weiss »

It is all about the shape of the mold. I was working with a potter. She gave me a bisqued face. I could set the glass balancing between the nose and the chin, such that it was at an angle. I fired slowly enough to make an excellent drape over, conforming to the face and spreading out flat on the shelf around the face. The catch was that both times I did this, the glass cracked, during the cool down, because the glass shrunk more than the ceramic mold. So, I made a rubber mold from the ceramic face, and cast a refractory face. I did the same setup, and got excellent results. The expansion characteristics of the refractory shape caused it to shrink more than the glass during cool down, leaving me glass that was easy to remove, and shaped just the way I wanted.
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Post Reply