Post by Felt Glass »

Anyone have technique for avoiding devit on float glass at 1600f?
hoknok
Posts: 61
Joined: Mon Nov 03, 2003 9:18 am
Location: Raised up North, living in the South

Post by hoknok »

Borax (20 mule team) mixed with water and spayed on the glass. To this date, I have not had any devit problems so far.
Felt Glass
Posts: 2
Joined: Tue Jan 27, 2004 8:25 pm

Devit

Post by Felt Glass »

Thanks Hoknok, I'll give it a try.
nancy burke
Posts: 1
Joined: Mon Jul 21, 2003 8:27 am
Location: Gloucester, On. Canada

Re: Float glass devitrification spray or other technique

Post by nancy burke »

Felt Glass wrote:Anyone have technique for avoiding devit on float glas
s at 1600f?


I use 'Clear Coat Overglaze" which is ideal for clear window
glass or plate
OR
Super Spray. Both these Fuse Master products come from Gil Reynolds
Fusion Headquarters. I consider both to be never-fails.