Need help with this schedule
Posted: Sat Jul 28, 2012 1:11 pm
I'm not sure if I should have put this in the newbie section or not but here goes.
I fused this flower using Spectrum96 the petals have one smaller piece of glass on top for extra strength. It fused flatter than what I really wanted and I had already adjusted my segment 4 down from 1475 to 1440. I am also using a brand new kiln.
I want to acheive a little dimension in the petal where the other piece of glass was but I want it smoother than the regular dimensional. Anyway I have 2 pictures and here is the Firing schedule I used. Would someone mind tweaking this for me as I am still quite new to this. I just want the middle of the petal a little bit more raised. Thanks for looking. Oh and just one last thing, when I first place the glass on the shelf all of the petals were touching each other they have really pulled away quite a bit so I am assuming it was too hot?
Seg Rate Targ Hold
1 300 900 15 min
2 500 1100 00
3 100 1250 30
4 9999 1440 10
5 9999 960 45
6 100 800 00
7 200 700 00
![Image](http://i.rwpic.com/images/charmy/flower.jpg)
![Image](http://i.rwpic.com/images/charmy/petal.jpg)
I fused this flower using Spectrum96 the petals have one smaller piece of glass on top for extra strength. It fused flatter than what I really wanted and I had already adjusted my segment 4 down from 1475 to 1440. I am also using a brand new kiln.
I want to acheive a little dimension in the petal where the other piece of glass was but I want it smoother than the regular dimensional. Anyway I have 2 pictures and here is the Firing schedule I used. Would someone mind tweaking this for me as I am still quite new to this. I just want the middle of the petal a little bit more raised. Thanks for looking. Oh and just one last thing, when I first place the glass on the shelf all of the petals were touching each other they have really pulled away quite a bit so I am assuming it was too hot?
Seg Rate Targ Hold
1 300 900 15 min
2 500 1100 00
3 100 1250 30
4 9999 1440 10
5 9999 960 45
6 100 800 00
7 200 700 00
![Image](http://i.rwpic.com/images/charmy/flower.jpg)
![Image](http://i.rwpic.com/images/charmy/petal.jpg)