Post by Michael Harmon »

I am consistently getting large bubbles when I do simple two layer pieces? I place a large solid piece on bottom with smaller elements on top. My schedule;

400 1225 20
600 1480 60
AFAP 900 60
100 700 0

Any suggestions would be greatly appreciated.
Michael Harmon
Posts: 9
Joined: Wed Apr 24, 2013 6:58 pm

Re: Bubble trouble

Post by Michael Harmon »

I tried to post a picture but I get an error message that says the file is too big.
Marty
Posts: 862
Joined: Mon Mar 10, 2003 3:58 pm
Location: Maine
Contact:

Re: Bubble trouble

Post by Marty »

Slow down on the way up. Try 300dph, or 250.
You're spending too much time at the top (at that temp).
Do some experiments- see what happens with 15 minutes at 1480, or 30 at 1460, etc. You'll have to find the right combo for your kiln/glass set up.
JestersBaubles
Posts: 705
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: Bubble trouble

Post by JestersBaubles »

are you capping with clear?

If so, Longer bubble squeeze.

Dana
Michael Harmon
Posts: 9
Joined: Wed Apr 24, 2013 6:58 pm

Re: Bubble trouble

Post by Michael Harmon »

Thanks Marty, I suspected that so I appreciate your confirmation. The piece just looked like it had gotten too hot. What do you think about this schedule;

400 1225 60
275 1460 10
AFAP 900 60
100 700 0
Valerie Adams
Posts: 587
Joined: Mon Apr 19, 2004 2:49 pm
Location: Santa Rosa, California
Contact:

Re: Bubble trouble

Post by Valerie Adams »

Is your lay up two full layers of glass? By that I mean, are the smaller pieces on top fitted together, or do you have areas of glass that is only one layer thick in places? That can cause bubbles.