Page 1 of 1
millefiorie
Posted: Sat Jul 22, 2017 5:17 pm
by jim simmons
Can anyone please give me an inkling on how to make millefiory
in the kiln?
Thanks in advance
The other Jim
Re: millefiorie
Posted: Sun Jul 23, 2017 4:46 pm
by Kevin Midgley
make your pattern using strips or rods of glass.
Can use a tin can initially to help hold them upright.
Once pattern is set, wire the rods and strips together on the outside.
I'd suggest using 6" or 15cm pieces.
Take them out of the can and place in the kiln vertically.
Preferably the kiln is top loading or the pick up on a punty is going to be pretty tricky.
Heat to tack fuse when you will pick them up and transfer them to a glory hole and then be able to pull them.
Make sure your power to the elements is off when working inside the kiln!!
Re: millefiorie
Posted: Mon Jul 24, 2017 12:09 am
by jim simmons
Thanks, Kevin
Re: millefiorie
Posted: Tue Jul 25, 2017 6:55 pm
by JenniferB
Here's a link to Cynthia Morgan's web site where she offers several murrine techniques.
<
http://www.morganica.com/glass/tools-su ... u-can-buy/>
Go to the bottom of the page where you'll find the information you're looking for.